What is the heat treatment process for electronic scale molds

Source:www.nmagri.com.cn      Release date: 2025-09-08
The heat treatment process of electronic scale molds needs to be combined with their core requirements - high dimensional stability (to avoid deformation affecting weighing accuracy), moderate hardness (to balance processability and wear resistance), low internal stress (to prevent long-term use cracking), and also need to be adapted to commonly used mold materials (such as pre hardened plastic mo
       The heat treatment process of electronic scale molds needs to be combined with their core requirements - high dimensional stability (to avoid deformation affecting weighing accuracy), moderate hardness (to balance processability and wear resistance), low internal stress (to prevent long-term use cracking), and also need to be adapted to commonly used mold materials (such as pre hardened plastic mold steel 718H, ordinary plastic mold steel P20, or 45 # steel for metal structural component molds). The following is a typical process flow and key link description:
1、 Core premise: Material selection and pre-processing
      Different materials correspond to different heat treatment schemes. Electronic scale molds are mainly "plastic molds" (such as shell and tray molds), with a few being metal structural component molds. Pre treatment is the foundation for ensuring stable subsequent processes
1. Material matching:
      Mainstream choice: 718H (pre hardened plastic mold steel) - has reached 28-32HRC at the factory, does not require overall quenching, only local aging strengthening is needed;
      Economic choice: P20/45 # steel - requires "quenching and tempering+surface hardening" to achieve performance, suitable for low precision, small batch molds.
2. Pre treatment (stress relief annealing):
      Purpose: To eliminate internal stress caused by forging/rough machining of mold blanks and avoid deformation during subsequent heat treatment;
      Process: Heat to 600-650 ℃, hold for 2-4 hours (depending on the mold size), slowly cool in the furnace to below 200 ℃, and remove from the furnace;
      Key: For complex cavities (such as anti slip patterns on electronic scale trays), an additional stress relief annealing is required after rough machining and before precision machining.
2、 Mainstream Process: Typical Heat Treatment Process by Material
1. Pre hardened steel (718H): local strengthening+stabilization treatment (most commonly used)
      The 718H has been pre hardened to 28-32HRC before leaving the factory, and does not require overall quenching (to avoid deformation of the mold cavity). Only the parts that are prone to wear (such as parting surfaces and gates) need to be strengthened and the processing stress eliminated
Step 1: Stress relief after rough machining
      Heat to 550-580 ℃, hold for 3 hours, then cool in the furnace to 300 ℃ and air cool out of the furnace (temperature below the critical point of Ac1 to avoid phase transition) to eliminate the stress generated by rough milling.
Step 2: Local surface hardening (optional)
      If the mold parting surface and gate require higher wear resistance (to prevent long-term opening and closing wear), low-temperature nitriding should be used:
      Temperature: 450-500 ℃, keep warm for 15-20 hours;
      Effect: A 5-15 μ m nitride layer is formed on the surface, with a hardness of 60-70HRC, and the core still maintains 28-32HRC (balancing toughness and preventing cracking).
Step 3: Stable aging after precision machining
      Precision machining of molds (after the completion of key dimensions such as cavities and positioning holes), heating to 500-520 ℃, holding for 4-6 hours, and slow cooling with the furnace;
      Purpose: To further stabilize the organization (reduce dimensional drift during subsequent use), while releasing precision machining stress, ensuring that the cavity size error of the electronic scale mold is ≤ 0.02mm after long-term use (meeting the assembly accuracy of weighing components).
2. Ordinary mold steel (P20/45 # steel): quenched and tempered+surface hardened (economical type)
      P20/45 # steel is not pre hardened and needs to be quenched and tempered to obtain basic strength, followed by surface strengthening to improve wear resistance. It is suitable for electronic scale shell molds with low precision requirements:
Step 1: Quenching and tempering treatment (overall performance improvement)
      Quenching: Heat to 830-860 ℃ (upper limit for P20, lower limit for 45 # steel), hold for 1-2 hours (depending on thickness), and cool with oil to room temperature;
      High temperature tempering: Heat to 580-620 ℃, hold for 2-3 hours, and air cool;
Effect: The hardness reaches 22-26HRC, the microstructure is composed of martensite, and it combines strength and machinability, laying the foundation for subsequent precision machining.
Step 2: Surface quenching (local wear-resistant strengthening)
      Induction heating surface quenching is used for vulnerable parts such as parting surfaces and gates
      Temperature: 900-950 ℃, rapid heating (to avoid phase transition in the core), water spray cooling;
      Effect: The surface hardness reaches 50-55HRC, the depth of the hardened layer is 0.5-1mm, and the core still maintains 22-26HRC (anti brittle fracture).
Step 3: Low temperature stress relief tempering
      After surface quenching, heat to 180-200 ℃, hold for 2 hours, and air cool;
Purpose: To eliminate internal stress caused by surface quenching and prevent cracking during mold use.
3、 Key control steps: avoiding deformation and ensuring accuracy
      The electronic scale mold has high requirements for dimensional accuracy (such as the coaxiality between the mold cavity and the installation position of the weighing sensor), and it is necessary to focus on controlling three aspects:
Heating rate:
      When heating large molds (such as electronic scale platform panel molds), the rate should be ≤ 100 ℃/hour to avoid thermal stress deformation caused by excessive temperature difference;
Cooling method:
       Pre hardened steel (718H): slow cooling or air cooling throughout the furnace, water cooling is prohibited (to prevent cracking);
       Ordinary steel quenching and tempering: oil cooling (45 # steel) or water-soluble quenching agent cooling (P20) after quenching to avoid deformation caused by too fast cooling rate;
Time stability:
       After precision machining, 1-2 aging treatments (500-520 ℃) must be carried out, and key dimensions must be measured after each insulation until the dimensions are stable (change ≤ 0.005mm).
4、 Process validation: performance testing
      After heat treatment, two core tests are required to ensure that the usage requirements are met:
Hardness testing:
      Core hardness: 28-32HRC required for 718H, 22-26HRC required for P20/45 # steel;
Surface hardening layer: After nitriding/quenching, it needs to reach 50-70HRC (depending on the location requirements);
Dimensional inspection:
      Use a coordinate measuring instrument to detect the size of the mold cavity and the position of the positioning hole, with an error of ≤ 0.02mm (to avoid affecting the assembly and weighing accuracy of the electronic scale).
久久亚州精品日韩| 亚洲色情中文字幕| 久草热久草在线视频| 国产一级a毛一级a看免费视频一| 亚洲午夜红桃福利网| 亚洲无码高清免费视频| 三级无码视频网址| 毛片在线观看一区| 91av亚洲视频| 黄色亚洲日韩欧美| 亚洲欧美州色色色色色色涩| 黄片毛片A级片| 日产精品欲AV麻豆| www99rea黄片大全| 日逼电影色情无码性爱小视频| 麻豆精品韩国三级| 欧美一级录像黄色影片| 亚洲激情播播91看黄片| 超碰海外福利导航| 欧美成人性生活A片手机版| 欧美黄色高清视频| 波多野结衣二区看黄片在线| 六月婷婷综合国产| 成人黄色在线久草资源站| 黄片视频1000秒试看| 无码内射人妻一级性交电影| 久草中文波多野结衣| 探花AV在线无码艺术三级片 | 中国一级成人无码片| 蜜臀久久久一区二区三区| 亚美黄色系列片子看看| 国产性爱无吗视频| 中美无码高清视频| 婷婷五月婷婷无码不卡av| 可以直接免费观看的黄色视频| 美国一级片免费视频| 日韩一级无码AV毛片观看| 国模在线私拍在线| 日韩第一区超碰在线| 外国一级a片中文字幕婷婷色 | 婷婷五月精品激情|